Views: 0 Author: Site Editor Publish Time: 2026-11-24 Origin: Site
An MPP foam compression curve shows the compressive stress generated as microcellular polypropylene foam is compressed by different percentages. Engineers use it to compare a candidate battery pad with the available cell gap and allowable contact pressure range.
Fuqiang's published MPP25 data provides compression stress ranges at 10% through 70% compression [1]. These values are useful for preliminary screening, but they do not establish long-term force retention or suitability for every battery cell design.
Fuqiang MPP25 published compression stress ranges. Source: Fuqiang MPP product page [1]. Specimen: 50 × 50 × 2 mm; published compression rate: 2 mm/min.
Compression Strain | Published Stress Range (MPa) | Engineering Interpretation |
|---|---|---|
10% | 0.11–0.24 | Initial compression response |
20% | 0.14–0.34 | Response at modest deflection |
30% | 0.17–0.38 | Intermediate compression response |
40% | 0.22–0.42 | Higher installed compression |
50% | 0.28–0.47 | Substantial compression load |
60% | 0.34–0.54 | High compression response |
70% | 0.44–0.67 | Very high deflection requiring specific evaluation |
These are manufacturer-published ranges, not nominal design targets, cell manufacturer limits, or universal MPP specifications. The published MPP25 density is 36 ± 5 kg/m³ [1].
An incorrect compression calculation can make a foam appear suitable even when it will exceed the cell's allowable mechanical loading.
Calculate compression from the pad's free thickness and the actual installed gap, including dimensional tolerances.
Compression percentage equals (free thickness minus installed thickness) divided by free thickness, multiplied by 100. For example, assuming a 2.0 mm pad is installed at 1.4 mm, the strain is 30%. Fuqiang's published MPP25 range at 30% is 0.17–0.38 MPa [1]. The calculated strain is an example, not an approved battery design condition.
A foam with excessive compressive stress can overload the cell, while insufficient force may fail to maintain intended contact during operation.
Compare the material stress range at each relevant compression state with the cell manufacturer's allowable pressure range.
Evaluate minimum and maximum assembly gaps, reversible cell swelling, and aging-related dimensional changes. Do not use one point on the curve to represent all conditions. The MPP25 data describes the reported specimen test conditions; temperature, rate, loading history, and finished pad dimensions may alter the observed response.
Confusing stress with force can lead to incorrect cell stack loading calculations.
Estimate force by multiplying compressive stress by the effective contact area, then verify the real part geometry.
For an illustrative 100 cm² pad at 30% compression, the reported MPP25 stress range of 0.17–0.38 MPa corresponds to approximately 1,700–3,800 N under an assumption of uniform pressure. This is a calculation example, not a validated force for a manufactured pad. Cutouts, edge effects, and nonuniform cell contact can change the actual force distribution.
A pad can meet its initial compression target but lose supporting force after prolonged operation.
Evaluate long-term stress relaxation and compression recovery separately from the initial stress-strain curve.
Compression set describes residual deformation after a defined compression and recovery procedure; stress relaxation describes force loss under sustained deformation. A short-duration compression curve cannot establish either property. Buyers should request relevant aging data and representative long-term tests at the intended battery temperature and compression.
Send the free pad thickness, installed gap range, allowable cell pressure, and cell swelling data for a material screening review. Request assessment of the available MPP25 data and any additional tests necessary for your design.
Is the MPP25 curve a recommended compression range for all battery packs?
No. It is published material test data. A suitable operating range depends on the individual cell and module design.
Can MPP25 compression stress be calculated from density alone?
No. Density does not uniquely define the material's stress-strain behavior.
Can you interpolate between published compression points?
Interpolation may support preliminary estimates, but it does not replace measured data or approval at the required condition.
Is 70% compression acceptable for a battery pad?
Not automatically. A high compression level requires confirmation of mechanical loading, recovery, material integrity, and long-term behavior.
Does an MPP foam compression curve prove thermal runaway protection?
No. Mechanical compression performance and thermal runaway barrier performance are separate requirements.
An MPP foam compression curve should be read against the actual battery gap, pressure limits, and expected dimensional changes. The published Fuqiang MPP25 data provides a useful starting point, but long-term and finished-part behavior still require validation.
Review the Fuqiang MPP25 product specifications. For a custom pad evaluation or quotation, provide the cell dimensions, allowed pressure range, free thickness, installed gap limits, and drawing. Request a comparison of the material data with your actual loading requirements.
Fuqiang Group, Microcellular Polypropylene Foam for EV Battery Applications — MPP25 Technical Data.
ASTM International, ASTM D3575 — Standard Test Methods for Flexible Cellular Materials Made from Olefin Polymers. Applicability must be confirmed for the tested product.
Fifteen years of automotive wire harness industry experience supports practical engineering decisions involving insulation materials, foam converting, dimensional control, and quality inspection. Battery compression components require grade-specific property evaluation and representative validation. Clear pressure requirements and drawings help customers move from material screening to defined sample specifications.